Unfiltered Methods (For Influence of Metal Powder Partiucle Geometry on Ultrasonically Embedded Nanocellulose Composites)

1 Mins read

Samples

  • 5 Powders (Copper, Iron, Bronze, Aluminium, Zinc)
  • Each series is for one powder and has 6 samples
  • Time sequence for each series: 5, 10, 20, 30, 45, 60 s
  • 0.5 cm³ of powder per sample
  • 5 cm³ of 10% SLS solution

Area Covered by Powder (%)

5 s 10 s 20 s 30 s 45 s 60 s
Aluminium 0.18 0.10 0.12 0.01 0.18 0.02
Bronze 0.02 0.04 0.06 0.03 0.03 0.00
Copper 9.31 46.28 15.07 7.20 8.41 11.88
Iron 0.16 0.29 0.31 0.26 0.38 0.02
Zinc 0.05 0.02 3.22 0.69 0.05 0.36